Injection Blow Molding General Processing Guidelines
| MATERIAL |
Zone 1 |
Zone 2 |
Zone3 |
Zone 4 |
Manifold (1) |
Melt |
Mold Temp |
| ABS |
380-500 |
390-510 |
400-520 |
400-540 |
400-540 |
400-540 |
110-200 |
| ACRYLIC |
360-470 |
370-480 |
380-490 |
390-510 |
400-510 |
400-510 |
130-220 |
| EVA |
320-420 |
320-430 |
330-440 |
340-460 |
340-460 |
340-460 |
40-120 |
| LDPE |
320-420 |
320-430 |
330-440 |
340-460 |
340-460 |
340-460 |
40-120 |
| HDPE |
350-460 |
360-470 |
370-480 |
370-500 |
380-500 |
380-500 |
40-140 |
| PAX PURGE (2) |
350-460 |
360-470 |
370-480 |
390-490 |
375-500 |
390-500 |
N/A |
| PBT |
400-460 |
400-470 |
410-480 |
420-490 |
430-490 |
440-490 |
60-160 |
| PETG |
440-500 |
450-500 |
460-510 |
470-520 |
470-520 |
480-520 |
60-120 |
| PC |
500-540 |
510-560 |
520-570 |
520-580 |
520-600 |
520-580 |
140-250 |
| PC/ABS |
420-510 |
430-520 |
440-540 |
450-550 |
440-580 |
450-550 |
120-200 |
| PP GENERAL PURPOSE |
350-470 |
360-480 |
370-490 |
380-500 |
380-500 |
380-500 |
40-140 |
| PS GENERAL PURPOSE |
350-450 |
360-460 |
370-470 |
380-480 |
390-480 |
390-480 |
70-200 |
| PS HIGH IMPACT |
350-450 |
360-460 |
370-470 |
380-480 |
390-480 |
390-480 |
70-200 |
| PVC FLEXIBLE |
300-390 |
300-390 |
310-390 |
320-400 |
320-400 |
320-390 |
50-150 |
| PVC RIGID |
280-370 |
300-380 |
320-390 |
330-400 |
340-400 |
350-410 |
50-140 |
| TPE (HYTREL (3) ) |
320-470 |
330-480 |
340-490 |
350-500 |
370-500 |
370-500 |
60-150 |
| TPE (SANTOPRENE (4) ) |
350-470 |
360-480 |
370-490 |
380-500 |
380-500 |
390-500 |
50-150 |
| TPO |
350-470 |
360-480 |
370-490 |
380-500 |
380-500 |
390-500 |
50-150 |
| TPR (ALCRYN (3) ) |
300-370 |
300-380 |
310-390 |
320-400 |
320-400 |
320-400 |
50-120 |
| TPU |
360-450 |
360-460 |
360-460 |
360-470 |
370-470 |
360-460 |
60-140 (A) |
| It may be necessary for die tip temperatures to be above or
below the listed range for head temperatures. Note: Check manufacturer’s
recommendations for specific processing temperatures. |
|
|